The glass lining on a Chinese reactor is a borosilicate enamel, broadly 60–75 % SiO2, 8–14 % B2O3, 3–6 % Al2O3 and under 10 % combined Na2O and K2O, fired at roughly 800–900 °C onto grit-blasted carbon steel. The blue-green colour is deliberate: cobalt oxide supplies the blue, copper or chromium oxide the green, and both are added so the coating can be identified and inspected. Colour is not what resists the acid — the silica network is — and two linings of identical hue can differ measurably in hot-alkali service life.
1. The oxide recipe, and what each part does
No mill publishes its full enamel recipe, and you should not expect one. What you can reasonably ask for is the oxide family and the ranges, which is enough to judge whether a grade is built for chemical duty or for something else.
- SiO2, 60–75 % — the network former. Acid resistance scales with it. Hydrofluoric acid and fluoride-bearing media attack this network directly, which is why no glass lining resists them.
- B2O3, 8–14 % — lowers thermal expansion and the firing temperature. It is why the lining can survive a 110 °C cold shock on a steel shell. Excess boron trades away water and alkali resistance.
- Al2O3, 3–6 % — raises chemical durability and hardness, at the cost of a stiffer melt that needs a longer firing cycle.
- Na2O and K2O, 5–10 % combined — fluxes. They are necessary to melt and bond the coating below 900 °C, and every extra point of alkali raises expansion and shortens acid life. Good grades run them as low as the firing window allows.
- CaO, MgO, ZnO, TiO2 — a few percent, used to modify the melt, opacify, or widen the firing window.
- Co3O4, CuO, Cr2O3 — under 1–2 % in total, and present for colour and nothing else.
2. Why borosilicate, and where the 110/120 °C figures come from
The published thermal shock limits for Chinese glass-lined reactors — cold shock ≤ 110 °C, heat shock ≤ 120 °C — are a direct consequence of the borosilicate system. B2O3 keeps the coefficient of expansion close enough to that of the steel beneath it that the two expand together across a normal heating or cooling cycle.
A soda-lime glass would be cheaper to melt and would craze on the first cold charge. That is the whole reason the industry settled on boron, and why a quotation that promises a thermal shock figure far above 120 °C without a change of lining grade should be treated as a typing error until proven otherwise.
Two coats are normal. A cobalt-bearing ground coat bonds to the steel; the cover coat carries the colour and the chemical duty. Thickness is quoted in millimetres on the mill's certificate — confirm the figure against your drawing rather than assuming a number.
3. Where the blue-green actually comes from
Base borosilicate enamel fired on steel is a translucent grey-green, not blue. The familiar blue-green is a mixed colourant system: cobalt oxide gives a deep blue, chromium or copper oxide shifts it toward green, and the balance between them sets the final hue. Iron picked up from the steel and the furnace atmosphere pushes the same recipe toward olive or grey.
That has a practical consequence. Hue is not tightly controlled, because it does not need to be. Vessels from the same mill, in the same order, can differ visibly in shade and both be correct.
Two linings the same colour are not the same lining, and two linings a slightly different colour are not a defect. Ask for a retained physical sample, not a colour description on a datasheet.
4. The colours you will see quoted in China
- Blue-green — the default for general chemical duty, and what most quotations assume when nothing is specified.
- Deep cobalt blue — a single-colourant variant used by some mills as their standard. Identical duty in most cases; ask for the certificate rather than inferring from the shade.
- White or opacified off-white — common on pharmaceutical and fine-chemical vessels. Dark star cracks, inclusions and product residue show up against it far more clearly than against a dark lining, which matters during inspection and cleaning verification.
- Black or dark grey — occasionally specified for light-sensitive products. It also hides defects, so pair it with a documented high-voltage test rather than a visual pass.
Colour is not a performance parameter on the datasheet. The datasheet lists design pressure in MPa, design and operating temperature in °C, lining thickness in mm, thermal shock limits and the high-voltage test in kV. Hue is not on it, and a supplier who leads with colour is steering the conversation.
5. Does colour correlate with corrosion resistance?
No. There is no accepted relationship between the hue of a glass-lined reactor and its resistance to a given medium. The colourant loading is under 1–2 % and sits in the glass network as an ion, not as a separate phase that a reagent can attack selectively.
What does decide service life is the ratio of network formers to fluxes, the thickness and coverage at welds, nozzle necks and the bottom knuckle, the bubble and void count in the fired coat, and whether the firing was complete. An underfired cover coat is more open chemically and will fail early whatever colour it is. Those are found by the high-voltage test and by sectioning a test coupon — not by eye.
The media limits are chemistry, not colour. Glass lining is not suitable for hydrofluoric acid or fluoride-bearing media, for phosphoric acid at 30 % or above and above 180 °C, or for strong alkali above pH 12 at 100 °C. No choice of blue, green, white or black changes any of those three lines.
There is one second-order link worth naming honestly. Opacifiers and colourants change melt viscosity and therefore the firing window, so a heavily opacified white enamel and a standard blue-green enamel from the same mill are not the same recipe. Their performance in hot alkali can differ. That difference has to be verified by test against your medium, not judged from a sample tile — and if the white grade is only offered on the pharmaceutical line, the cost difference is real.
6. What colour is genuinely useful for
Three things, all of them commercial rather than chemical. It identifies the mill and the grade, which is how you catch a substituted vessel at the factory gate. It makes chip and crack inspection faster, in opposite ways: a white lining shows dark cracks, a dark lining shows bright chips. And a recorded shade, agreed against a retained sample, gives you a batch-consistency check across repeat orders without opening the vessel.
Write it into the specification as a line — colour and gloss to an approved sample retained by both parties — and it becomes a real acceptance criterion instead of a conversation.
7. What to put on the enquiry
- Media list with concentration and maximum operating temperature in °C, so the grade can be matched to the chemistry rather than to the colour.
- Required thermal shock limits, stated as cold shock and heat shock in °C.
- Lining thickness in mm, high-voltage test in kV, and a copy of the mill's inspection record for both.
- Colour, as an approved physical sample, with the sample retained by both sides.
- A statement of the enamel type — borosilicate chemical-duty grade — even if the full oxide recipe stays proprietary.
Takeaway
Treat the blue-green as paint with a job: it identifies the supply and helps you inspect. Treat the borosilicate chemistry, the thickness in mm, the thermal shock figures in °C and the high-voltage test in kV as the things that decide whether the vessel is still in service in ten years.